Protecto 401 Ceramic EpoxyProtecto 401 Ceramic Epoxy
CALL TOLL FREE 1-888-SPEC401 or Email

COMPARISON TESTS

Protecto 401 vs. Polyamide Coal Tar Epoxy

TEST PROTECTO 401 POLYAMIDE COAL
TAR EPOXY

PERMEABILITY
Procedure "A"
of ASTM E-96-66
42 Day Test Duration
0.00 perms .22 perms
Note: The lower the permeability rating the less water borne chemicals can penetrate the lining.
IMMERSION
in 20% sulfuric acid
No blisters or de-
lamination of lining
after 24 months.
Blisters over all of the tested area of lining after 3 months. Test terminated.
Note: (Rated using standards according to ASTM D714-87 Evaluating the degree of blistering).
SALT SPRAY
5% solution
ASTM B 117-85
Scribed
24 months
No undercutting at
scribe. No damage
to panel.
After 4.7 months no
undercutting at scribe. No
damage to panel

Note: All materials were tested with an average film thickness of 40 mils.

Back to Table of Contents

CALL TOLL FREE 1-888-SPEC401 or Email

Logos and pictures shown are trademarks of their respective owners
Copyright © 2000, Digital Trends Corporation