Protecto 401 Ceramic EpoxyProtecto 401 Ceramic Epoxy
CALL TOLL FREE 1-888-SPEC401 or Email

COMPARISON TESTS

Protecto 401 vs. Polyethylene

TEST
PROTECTO 401 RESULTS
POLYETHYLENE RESULTS

  1.  160°F DISTILLED
       WATER IMMERSION

       scribed panels
       Rated using ASTM
       D-714-87
24 months, slight red
rust in scribe, no
undercutting.
1-1/2 months, delamination
of film, test terminated.

  2.  120°F TAP WATER
       IMMERSION

       scribed panels
       Rated Using ASTM
       D-714-87
24 months, slight red rust
in scribe, no undercutting.
6 months, film curls
back l/2" from scribe,
test terminated.

  3.  140°F 25% SODIUM
       HYDROXIDE
       IMMERSION

       Rated Using ASTM
       D-714-87
24 months, no effect. 1-1/2 months, delamination
of film, test terminated.
unscribed

  4.  SALT SPRAY
       ASTM B-117
       scribed panels
24 months, red rust in scribe,
no undercutting.
1-1/2 months, l-1/2" under-
cutting at scribe. Test
terminated
Note: All materials were tested with an average film thickness of 40 mils on production-run ductile iron pipe.